Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® Advanced T2300HG6 LS sw23346 - PA6T/66-GF30 - BASF

Material Data Center offers the following functions for Ultramid® Advanced T2300HG6 LS sw23346:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Heat stabilized, partially aromatic polyphthalamide for injection molding with strong mechanical properties especially at elevated temperatures and good chemical resistance for highly stressed parts. The product can be characterized as compound with high strength and stiffness. It features a high melting point (310°C) and good heat resistance.

Markets & applications
Automotive: sensors, e-mobility
E&E: Connectors
Consumer goods
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 5 / * cm³/10min ISO 1133
Temperature 320 / * °C -
Load 5 / * kg -
Molding shrinkage, parallel 0.5 / * % ISO 294-4, 2577
Molding shrinkage, normal 1.1 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 10400 / 10200 MPa ISO 527
Stress at break 190 / 160 MPa ISO 527
Strain at break 2.8 / 3 % ISO 527
Flexural modulus, 23°C 9300 / 9300 MPa ISO 178
Flexural strength 270 / 240 MPa ISO 178
Charpy impact strength, +23°C 90 / 75 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 65 / 55 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 8.5 / 8.1 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 7.5 / 7.1 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 310 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 280 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 280 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 22 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 72 / * E-6/K ISO 11359-1/-2
Burning behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.4 / * mm -
Electrical propertiesdry / condUnitTest Standard
ISO Data
Relative permittivity, 1MHz 3.8 / 4 - IEC 62631-2-1
Dissipation factor, 1MHz 170 / 270 E-4 IEC 62631-2-1
Volume resistivity >1E13 / >1E13 Ohm*m IEC 62631-3-1
Surface resistivity * / >1E15 Ohm IEC 62631-3-2
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 4.2 / * % Sim. to ISO 62
Humidity absorption 1.32 / * % Sim. to ISO 62
Density 1390 / - kg/m³ ISO 1183
Bulk density 700 kg/m³ -
Material specific propertiesdry / condUnitTest Standard
ISO Data
Viscosity number 130 / * cm³/g ISO 307, 1157, 1628
Diagrams
Viscosity-shear rate , Ultramid® Advanced T2300HG6 LS sw23346, PA6T/66-GF30, BASF
Shearstress-shear rate , Ultramid® Advanced T2300HG6 LS sw23346, PA6T/66-GF30, BASF
Stress-strain , Ultramid® Advanced T2300HG6 LS sw23346 (dry), PA6T/66-GF30, BASF
Stress-strain , Ultramid® Advanced T2300HG6 LS sw23346 (cond.), PA6T/66-GF30, BASF
Secant modulus-strain , Ultramid® Advanced T2300HG6 LS sw23346 (dry), PA6T/66-GF30, BASF
Secant modulus-strain , Ultramid® Advanced T2300HG6 LS sw23346 (cond.), PA6T/66-GF30, BASF
Tensile modulus-temperature , Ultramid® Advanced T2300HG6 LS sw23346 (dry), PA6T/66-GF30, BASF
Tensile modulus-temperature , Ultramid® Advanced T2300HG6 LS sw23346 (cond.), PA6T/66-GF30, BASF
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets, Black
Additives
Lubricants
Special Characteristics
Heat stabilized or stable to heat
Chemical Resistance
General Chemical Resistance
Applications
Automotive, Electrical and Electronical
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .05 %
Pre/Post-processing, Pre-drying, Temperature: 120 °C
Pre/Post-processing, Pre-drying, Time: 8 h

PROCESSING
injection molding, Melt temperature, range: 320 - 340 °C
injection molding, Melt temperature, recommended: 330 °C
injection molding, Mold temperature, range: 120 - 160 °C
injection molding, Mold temperature, recommended: 140 °C
injection molding, Dwell time, thermoplastics: 5 min
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com